Synthesis
In2O3 + 2H2 = In2O +
2H2O
In the method of Klemm and Von Vogel, as developed by Thiel
and Luckmann, In2O3 is reduced with H2 at a temperature less
than 400°C until the reduction product acquires a composition approximating Ing O (overreduction results in partial conversion to
metallic In). The reduction product is then vacuum-sublimed from
a corundum boat in quartz apparatus and collected on a cold finger.
The temperature must be so selected that the outside surface of
the sublimator is no higher than about 750°C, since decomposition
of sublimed In2O sets in at higher temperatures.